Iron - Density, Specific Heats and Thermal Conductivities vs. Temperatures

Sponsored Links
Iron - Density, Specific Heats and Thermal Conductivities vs. Temperatures
T
(K)
ρ
(kg/m³)
c
(kJ/kg K)
k
(W/m K)
100 7900 0.216 134
150 7890 0.324 104
200 7880 0.384 94
250 7870 0.422 87
300 7860 0.450 80
400 7830 0.491 70
600 7760 0.555 55
800 7690 0.692 43
1000 7650 1.034 32
1200 7620 28
1400 7520 31
1600 7420
1800 7420
Sponsored Links

Related Topics

Material Properties

Properties of gases, fluids and solids. Densities, specific heats, viscosities and more.

Related Documents

Cast Iron

The four basic types of cast iron - white iron, gray iron, ductile iron and malleable iron.

Cast Iron Soil Pipes - Dimensions

Dimensions of cast iron soil pipes.

Copper, Ductile Iron, Carbon Steel, Stainless Steel and Aluminum Piping Materials - Temperature Expansion

Thermal expansion of typical piping materials.

Metals - Latent Heat of Melting

Metals and their latent heat of fusion.

Metals - Specific Heats

Specific heat of commonly used metals like aluminum, iron, mercury and many more - imperial and SI units.

Metals - Temperature Expansion Coefficients

Thermal expansion coefficients metals.

Metals and Alloys - Densities

Densities of some common metals, metallic elements and alloys - aluminum, bronze, copper, iron and more.

Metals and Alloys - Young's Modulus of Elasticity

Elastic properties and Young's modulus for metals and alloys like cast iron, carbon steel and more.

Metals Strength vs. Temperature

The influence of temperature on the strength of metals.

Thermal Conductivity of Metals and Alloys: Data Table & Reference Guide

Thermal conductivities of common metals, metallic elements and alloys.

Sponsored Links

Search Engineering ToolBox

Search is the most efficient way to navigate the Engineering ToolBox!

SketchUp Extension - Online 3D modeling!

Add standard and customized parametric components - like flange beams, lumbers, piping, stairs and more - to your Sketchup model with the Engineering ToolBox - SketchUp Extension - enabled for use with the amazing, fun and free SketchUp Make and SketchUp Pro . Add the Engineering ToolBox extension to your SketchUp from the Sketchup Extension Warehouse!

Privacy

We don't collect information from our users. Only emails and answers are saved in our archive. Cookies are only used in the browser to improve user experience.

Some of our calculators and applications let you save application data to your local computer. These applications will - due to browser restrictions - send data between your browser and our server. We don't save this data.

Google use cookies for serving our ads and handling visitor statistics on the AMP pages. Please read Google Privacy & Terms for more information about how you can control adserving and the information collected.

AddThis use cookies for handling links to social media. Please read AddThis Privacy for more information.