PVC Polyvinyl Chloride - Chemical Resistance

Sponsored Links

Chemical resistance of PVC - Polyvinyl Chloride - to common products is indicated in the table below.

  • R = resistant up to 60 oC (140 oF)
  • R23 = resistant up to 23 oC (73 oF)
  • N = not resistant
PVC Polyvinyl Chloride - Chemical Resistance
Chemical ProductResistance
Acetic Acid 0-25% (vinegar) R
Acetic Acid 25-50% R23
Alcohol - Butyl R
Alcohol - Isopropyl R
Alum (Aluminum Sulfate) R
Aluminum Chloride, Aqueous R
Aluminum Potassium Sulfate R
Ammonium Bisulfide R
Ammonium Hydroxide 10%

R

Ammonium Nitrate R
Ammonium Persulfate R
Ammonium Phosphate R
Ammonium Sulfate R
Barium Carbonate R
Barium Chloride R
Barium Sulfate R
Barium Sulfide R
Beer R
Benzene N
Benzoic Acid R
Benzyl Alcohol N
Butyric Acid 0-50% R23
Cadmium Cyanide R
Calcium Bisulfide N
Calcium Carbonate R
Calcium Chlorate R
Calcium Chloride R
Calcium Hydroxide R
Calcium Hypochlorite R
Calcium Nitrate R
Calcium Sulfate R
Carbon Dioxide R
Carbon Monoxide R
Carbonic Acid R
Chlorine - 0-20 ppm R23
Chlorine, liquid N
Chlorinated Water R
Chloroacetic Acid 0-50% R
Citric Acid R
Coconut Oil R
Coffee R
Coke Oven Gas R
Copper Chloride R
Copper Cyanide R
Copper Fluoride R
Copper Nitrate R
Copper Sulfate R
Corn Oil R
Corn Syrup R
Cottonseed Oil R
Crude Oil R
Cyclohexane N
Diesel Fuel R
Dioctyl Phthalate N
Dipropylene Glycol R
Ethylene Glycol R
Fatty Acids R
Ferric Chloride R
Ferric Nitrate R
Ferric Sulfate R
Ferrous Chloride R
Ferrous Nitrate R
Ferrous Sulfate R
Fish Oil R
Fluoboric Acid R
Fluorsilicic Acid 30% R
Formaldehyde R
Formic Acid R23
Fuel JP-4,5 R
Gas, Natural R
Gasoline R
Gasohol R
Gasoline, Sour R
Glycol, Acid R
Glucose R
Glycerin R
Glycol R
Glycolic Acid R
Heptane R
n-Hexane R23
Hydraulic oil (petroleum) R23
Hydrobromic Acid 20% R
Hydrocyanic Acid R
Hydrofluoric Acid R23
Hydrogen R
Hydrogen Cyanide R
Hydrogen Fluoride N
Hydrogen Peroxide 50% R
Hydrogen Sulfide Dry, Wet R
Hypochlorous Acid R
Iodine I2 N
Kerosene R
Lactic Acid 25% R
Lead Acetate R
Magnesium Carbonate R
Magnesium Chloride R
Magnesium Nitrate R
Magnesium Sulfate R
Malic Acid R
Mercuric Chloride R
Mercurous Nitrate R
Methane R
Methanol R
Milk R
Mineral Oil R
Motor Oil R
Naphtha R
Naphthalene R
Nickel Chloride R
Nickel Nitrate R
Nickel Sulfate R
Nicotine R
Nitric Acid R
Nitro Benzene N
Nitro Glycerine N
Oleic Acid R
Olive Oil R
Oxalic Acid 50% R
Phosphoric Acid R
Picric Acid, Alcoholic N
Potassium Aluminum Sulfate R
Potassium Bicarbonate R
Potassium Carbonate R
Potassium Chloride R
Potassium Ferrocyanide R
Potassium Nitrate R
Potassium Permanganate 10% R
Potassium Persulfate R
Potassium Sulfate R
Pyridine N
Silver Nitrate R
Soaps R
Sodium Acetate R
Sodium Benzoate R
Sodium Bisulfate R
Sodium Bisulfite R
Sodium Bromide R
Sodium Carbonate R
Sodium Chlorate R
Sodium Chloride R
Sodium Chlorite N
Sodium Cyanide R
Sodium Dichromate R
Sodium Phosphate R
Sodium Ferricyanide R
Sodium Hydroxide R
Sodium Hypochlorite R23
Sodium Meta-Phosphate R
Sodium Nitrate R
Sodium Silicate R
Sodium Sulfate R
Sodium Sulfide R
Sodium Sulfite R
Sodium Thiosulfate R
Stannic Chloride R
Stannous Chloride R
Stearic Acid R
Sugar, Sucrose R
Sulfamic Acid N
Sulfuric Acid 0-80% R
Sulfuric Acid 90% R23
Sulfuric Acid > 93% N
Sulfurous Acid R
Tall Oil R
Tannic Acid R
Tartaric Acid R
Toluene (Toluol) N
Transformer Oil R
Trichloroacetic Acid 50% R
Trisodium Phosphate R
Urea R
Vegetable Oils R
Vinegar R
Water - Deionized R
Water - Demineralized R
Water - Distilled R
Water - Fresh R
Water - Salt R
Water - Sea R
White Liquor - Pulp Mill R
Wine R
Xylene (Xylol) N
Zinc Chloride R
Zinc Nitrate R
Zinc Sulfate R
Sponsored Links

Related Topics

Material Properties

Properties of gases, fluids and solids. Densities, specific heats, viscosities and more.

Related Documents

CPVC - Chemical Resistance

Chemical resistance of CPVC - Chlorinated Poly (Vinyl Chloride) - to common chemicals and products.

Epoxy - Chemical Resistance

Chemical resistance of Epoxy to common products like Acetic acid, Alcohol, Diesel oil and more.

PE Polyethylene - Chemical Resistance

Chemical resistance of Polyethylene - PEH - to common products.

Polyurethane - Chemical Resistance

Chemical resistance of Polyurethane (PUR).

PP Polypropylene - Chemical Resistance

Chemical resistance of Polypropylene - PP - to acids, bases, organic substances and solvents.

Rubbers and Elastomers - Chemical Resistance

Rsistance to chemicals - solvents and softeners - swelling properties.

Silicone - Chemical Resistance

Chemical resistance of silicone.

Vinyl Ester - Chemical Resistance

Chemical resistance of Vinyl Ester to products as Acetone, Alcohol, Diesel oil and more.

Sponsored Links

Search Engineering ToolBox

Search is the most efficient way to navigate the Engineering ToolBox!

SketchUp Extension - Online 3D modeling!

Add standard and customized parametric components - like flange beams, lumbers, piping, stairs and more - to your Sketchup model with the Engineering ToolBox - SketchUp Extension - enabled for use with the amazing, fun and free SketchUp Make and SketchUp Pro . Add the Engineering ToolBox extension to your SketchUp from the Sketchup Extension Warehouse!

Privacy

We don't collect information from our users. Only emails and answers are saved in our archive. Cookies are only used in the browser to improve user experience.

Some of our calculators and applications let you save application data to your local computer. These applications will - due to browser restrictions - send data between your browser and our server. We don't save this data.

Google use cookies for serving our ads and handling visitor statistics on the AMP pages. Please read Google Privacy & Terms for more information about how you can control adserving and the information collected.

AddThis use cookies for handling links to social media. Please read AddThis Privacy for more information.