Aluminum - Thermophysical Properties

Density, specific heat and thermal conductivity related to temperature.

Aluminum - Thermophysical Properties
T
(K)
ρ
(kg/m³)
c
(kJ/kg K)
k
(W/m K)
150 2726 0.683 250
200 2719 0.797 237
250 2710 0.859 235
300 2701 0.902 237
400 2681 0.949 240
600 2639 1.042 231