Copper - Density, Specific Heat and Thermal Conductivity vs. Temperature

Density, specific heat and thermal conductivity of copper vs. temperature

Copper - Density, Specific Heat and Thermal Conductivity vs. Temperatures
T
(K)
ρ
(kg/m³)
c
(kJ/kg K)
k
(W/m K)
100 9009 0.254 480
150 8992 0.323 429
200 8973 0.357 413
250 8951 0.377 406
300 8930 0.386 401
400 8884 0.396 393
600 8787 0.431 379
800 8642 0.448 366
1000 8568 0.446 352
1200 8458 0.480 339