Engineering ToolBox - Resources, Tools and Basic Information for Engineering and Design of Technical Applications!

Permeability

Electromagnetism and formation of magnetic fields.

Permeability is the ability to support formation of magnetic fields in a material.

Permeability is measured in H/m (henries/m) or newtons/ampere2(N/A2) .

The Permeability of Free Space

The permeability of free space µ0 (the permeability constant or the magnetic constant) is

µ0 = 4π 10-7 (H/m)

≈ 1.257×10-6 (H/m, N/A2)

The Relative Permeability

The relative permeability is the ratio of the permeability of a specific medium to the permeability of free space µ0

µr = µ / µ0                      (1)

where

µr = relative permeability

µ = permeability of the medium (H/m)

The lowest relative magnetic permeability of a paramagnetic material is 1.0 - and the magnetic response of the material is the same as 'free space' or complete vacuum.

Substances - Permeabilities
MediumPermeability
- µ -
(H/m)
Relative permeability
- μ / μ0 -
Air 1.25663753×10-6 1.00000037
Aluminum 1.256665×10-6 1.000022
Austenitic stainless steel1) 1.260×10-6 - 8.8×10-6 1.003 – 7
Bismuth 1.25643×10-6 0.999834
Carbon Steel 1.26×10-4 100
Cobalt-Iron (high permeability strip material) 2.3×10-2 18000
Copper 1.256629×10-6 0.999994
Ferrite (nickel zinc) 2.0×10-5 – 8.0×10-4 16 – 640
Ferritic stainless steel (annealed) 1.26×10-3 - 2.26×10-3 1000 – 1800
Hydrogen 1.2566371×10-6 1
Iron (99.8% pure) 6.3×10-3 5000
Iron (99.95% pure Fe annealed in H) 2.5×10-1 200000
Martensitic stainless steel (annealed) 9.42×10-4 - 1.19×10-3 750 – 950
Martensitic stainless steel (hardened) 5.0×10-5 - 1.2×10-4 40 – 95
Nanoperm 1.0×10-1 80000
Neodymium magnet 1.32×10-6 1.05
Nickel 1.26×10-4 - 7.54×10-4 100 – 600
Permalloy 1.0×10-2 8000
Platinum 1.256970×10-6 1.000265
Sapphire 1.2566368×10-6 0.99999976
Superconductors 0 0
Teflon 1.2567×10-6 1
Vacuum 0) 4π 10-7 1
Water 1.256627×10-6 0.999992
Wood 1.25663760×10-6 1.00000043

1) Permeability of austenitic stainless steels is not like ferritic, martensitic and duplex stainless steel. Austenitic steel can be classed as paramagnetic with relative permeability approaching 1.0 in the fully austenitic condition. The low permeability enables austenitic steel to be used where a non-magnetic material is required.